GMW14872
An accelerated laboratory corrosion test to evaluate automotive coatings and components.
Introduction
In 2003 the American Iron and Steel Institute, in conjunction with a Committee of the SAE, conducted a study of existing cyclic corrosion tests in order to establish the best methods of predicting the performance of materials used in automotive applications. Twenty established corrosion test procedures were included within the study. The process itself comprised of undertaking tests on 10 different materials with each procedure, the results were compared to results gathered through real World exposure from 10 locations around the globe, undertaking the tests with identical materials.
The procedures were judged on:
- Their ability to replicate the rank order of coatings performance in the real World.
- Their ability to replicate the same type of failure as viewed in the real World
- Repeatability over multiple tests
- Speed
- Cost effectiveness
The test established that the General Motors standard GM9540P, was one of the best methods of cosmetic corrosion prediction of cold rolled steel and resulted in the publication of it’s successor GMW14872.
Test Conditions
The test method is composed of approximay 1% NaCL, CaCL2 and NaHCO3 salt mist applications combined with high temperature and humidity drying cycles, a single cycle of the test lasts for approximay 24 hours.
Method
Specimens being tested are exposed to a multi-stage changing environment that is composed of three distinctive cycles, these stages can be varied depending on the nature of the specimen undertaking the test, for further information please refer to the full GMW14872 standard.
The individual cycles comprise of
- An exposure of 8 hours to an ambient climate of between 40 and 50RH% at a temperature of +25C. During this period salt solution is sprayed directly on to the test samples 4 times, for long enough to thoroughly wet them. A minimum of 1 hour spacing between the end of a previous salt application and the following salt application is required. Collection rates for each 80 cm2 of horizontal collection area should be in the range of 0.75 mL/h to 1.5 mL/h.
- An exposure of 8 hours to a water fog humidity climate of 100%RH at a temperature of +49C.
- An exposure of 8 hours to air drying in a climate of <30%RH at a temperature of +60C.
The test length is variable dependant on the number of cycles within the total test duration.
Typical Application
Through analysis of historic data it has been determined that the GMW14872 test process very closely predicts the corrosion rates for steel and zinc materials exposed to periodic de-icing salts, for this reason the standard has become very popular within the automotive industry.
Additionally the US military regularly uses the standard to predict life of a variety of coatings and materials on tactical vehicles.
免責聲明
- 凡本網注明“來源:化工儀器網”的所有作品,均為浙江興旺寶明通網絡有限公司-化工儀器網合法擁有版權或有權使用的作品,未經本網授權不得轉載、摘編或利用其它方式使用上述作品。已經本網授權使用作品的,應在授權范圍內使用,并注明“來源:化工儀器網”。違反上述聲明者,本網將追究其相關法律責任。
- 本網轉載并注明自其他來源(非化工儀器網)的作品,目的在于傳遞更多信息,并不代表本網贊同其觀點和對其真實性負責,不承擔此類作品侵權行為的直接責任及連帶責任。其他媒體、網站或個人從本網轉載時,必須保留本網注明的作品第一來源,并自負版權等法律責任。
- 如涉及作品內容、版權等問題,請在作品發表之日起一周內與本網聯系,否則視為放棄相關權利。